Constantan wire technical parameters

Aug 30, 2021

Main technical properties of Constantan, New Constantan (Constantan wire), copper-manganese resistance alloy (GB/T1234-95 standard):

Performance  /  grade


Constantan 6J40


New Constantan 6J11


Manganese 6J12


F1 manganese copper 6J8


F2 manganese copper 6J13


 


Main chemical composition%


Ni


39-41


__


2-3


___


2-5


Mn


1-2


10.5-12.5


11-13


8-10


11-13


Cu


margin


margin


margin


margin


margin


other


__


Al:2.5-4.5

Fe:1.0-1.6


__


Si:1-2


__


Component applicable temperature ℃


5-500


5-500


5-45


10-80


10-80


Density g/m3


8.88


8.00


8.44


8.70


8.40


Resistivity.m, 20℃


0.48±0.03


0.48±0.03


0.46±0.03


0.35±0.05


0.44±0.04


Temperature Coefficient of Resistance

aí10-6/℃


+40

-40


+80

-80


+20

-3


+10

-5


40


Thermal electromotive force for copper

V/℃(0-100℃)


45


2


1


2


2


Elongation% (>0.5)


≥15


≥15


≥15


≥15


≥15


organization


Austenite


Austenite


Austenite


Austenite


Austenite


magnetic


Non-magnetic


Non-magnetic


Non-magnetic


Non-magnetic


Non-magnetic


Send Inquiry